Discover our innovative vacuum bonding technology that expertly combines PVC film with glued fiberboard. This advanced process allows for the seamless covering of a variety of decorative elements, including flat surfaces, concave and convex grooves, curved edges, and intricate hollow carvings. As a leading factory and supplier in China, we ensure that our vacuum forming technique is not only straightforward but also cost-effective. This makes it an ideal choice for the production of furniture, including paint-free doors, sliding doors, cabinets, and more. Elevate your furniture designs with our high-quality solutions and experience the benefits of our reliable manufacturing expertise

    Vacuum Forming Overview & Applications

    Use vacuum to bond the PVC film to the glued fiberboard to achieve the effect of covering various types of decorative parts such as flat surfaces, concave and convex grooves, curved edges, hollow carvings, etc.

    The vacuum forming process is simple and the production cost is low. It is widely used in the manufacture of furniture such as paint-free doors, sliding doors, cabinets, etc.

    Common Problems & Reference Solutions

    Issue 01 Poor Spraying (Glue breaking, spray gun clogging, etc.)
    Possible Reasons
    1. The viscosity of the plastic suction is too high.
    2. Dust and other particulate impurities are mixed into the plastic suction, or the skin is formed by itself, causing the spray gun to be blocked.
    Reference Solution
    1. Adjust the plastic suction formula, reduce the amount of thickener, and lower the viscosity of the plastic suction.
    2. Re-filter the plastic suction with a 200-mesh filter.
    Issue 02 Spraying Atomization is Too Small or Too Scattered

    Good atomization effect can help the plastic suction droplets to be more evenly dispersed, which is helpful for the board surface effect; but sometimes, the atomization effect is too good, and the plastic suction spray area will become very large, which is not conducive to the spraying of fine parts.

    Vacuum forming spray atomization analysis
    Possible Reasons
    1. The spray gun is not adjusted to the appropriate state.
    2. The viscosity of the plastic suction is not adjusted to the appropriate range.
    3. The rheological state of the plastic suction is not adjusted well.
    Reference Solution
    1. Adjust the spray gun to increase or decrease the atomization effect.
    2. Lowering the viscosity of the blister glue can improve the atomization effect; increasing the viscosity of the blister glue can reduce the atomization effect.
    3. Without changing the viscosity, the atomization effect can also be improved by selecting different thickeners to adjust the rheological state of the blister glue. Reducing the viscosity under high shear can improve the atomization effect; increasing the viscosity under high shear can reduce the atomization effect.
    Issue 03 After Spraying, the Board Surface Takes a Long Time to Dry
    Possible Reasons
    1. The glue film is sprayed too thick, resulting in the surface of the glue layer being filmed, while the internal moisture is difficult to evaporate.
    2. Environmental influence (such as low temperature and high humidity).
    3. Adding too much water to the blister glue formula system to adjust the solid content, or adding too much wetting and leveling agent may also slow down the drying speed.
    Reference Plan
    1. Spray evenly and reduce the amount of glue appropriately according to application requirements.
    2. Environmental factors are the most uncontrollable, and it is recommended to extend the waiting time appropriately; you can also place the fiberboard in a high temperature and ventilated place to help its moisture evaporate.
    3. Check the formula system of the blister glue and adjust it within the application requirements.
    Issue 04 Defects Such as Orange Peel or Pitting on the Board Surface After Film Drying
    Possible Reasons
    1. The spray gun is not adjusted properly (the atomization effect is not good during spraying).
    2. The viscosity of the blister glue is too high and the fluidity is not good.
    3. The state of the blister glue system is not well prepared.
    Reference Plan
    1. Adjust the spray gun to adjust the atomization effect to the appropriate state.
    2. The blister glue system is adjusted to the appropriate viscosity and rheological state, and supplemented with an appropriate amount of wetting and leveling agent to improve the surface effect.
    3. After the film is dried, gently polish it with fine sandpaper.
    (If necessary, please contact us, we will recommend a suitable thickener solution for you according to the actual application needs)
    Issue 05 After Vacuuming, PVC Film in the Groove Cannot be Sucked Down or Firmly Attached
    Possible Reasons
    1. The vacuum degree of the blister machine cannot be reached.
    2. When vacuuming, the four sides of the groove are tightly fitted together, so that the air inside the groove cannot be extracted.
    Reference Plan
    1. Check whether there is a problem with the blister machine.
    2. When spraying the blister glue, try not to spray too thickly around the groove.
    3. If conditions permit, opening 1~2 holes at the bottom of the groove can effectively solve this problem.
    Issue 06 After Decompression: Groove Rebounds & Outlines Become Unclear

    After decompression, the PVC film in the groove slowly rebounds, and the outline of the decorative parts gradually becomes unclear (on the same day or the next day).

    Note: After decompression, if the PVC film is not firmly attached, the later hand-tear strength and heat resistance will be affected.
    Possible Reasons
    1. The blister temperature is not enough, and the film cannot be activated well.
    2. The board surface temperature is still very high during decompression, and the initial strength of the blister glue cannot be well established; at this time, the blister glue with poor heat resistance is more likely to rebound.
    Reference Plan
    1. Appropriately increase the temperature of the blister machine or extend the blister time to allow the film to be fully activated (the film layer temperature should be kept above 55°C as much as possible).
    2. Especially in hot summer weather, the temperature of the board surface drops very slowly. You can use electric fans to blow directly or wipe with cold water to cool the board surface before removing the pressure.
    3. For the blister glue formula, you can choose a resin with better heat resistance and appropriately increase the proportion of resin in the formula system.
    Issue 07 After Unloading, Edge is Not Firm or Edge is Unsealed (Same Day or Next Day)
    Reference Plans & Analysis
    1. Activation check: Tear off the edge and observe that a continuous film can be formed on the side of the fiberboard, but there is no stickiness with the PVC film, then you need to consider the activation problem.
      Appropriately increase the temperature of the blister machine or extend the blister time to allow the film to be fully activated (the temperature of the side film layer should also be kept above 55°C as much as possible). If the temperature cannot be increased, adding 2~3% of tackifying resin to the blister glue formula system can sometimes partially improve the problem.
    2. Strength & Heat Resistance check: Tear off the edge, the film is on both sides of the fiberboard and the PVC film, but there is no bonding strength, considering the initial strength or heat resistance is not enough.
      Cool the board surface by direct fan blowing and wiping with cold water before removing the pressure. For the formula of blister glue, you can choose a resin with better heat resistance and appropriately increase the proportion of resin in the formula system.
    Issue 08 Grooves Rebound & Edge Glue Opens During Later Storage Process
    Possible Reasons

    On the premise of confirming that the initial blister is intact, it may be caused by high ambient temperature and insufficient heat resistance.

    Reference Plan
    1. Choose a resin with better heat resistance and appropriately increase the proportion of resin in the formula system.
    2. Adding 2~5% curing agent to the blister glue can effectively improve the heat resistance.
      Note: The curing agent should be prepared and used immediately, and it is recommended to use it when the heat resistance requirement is high.

    Frequently Asked Questions (FAQ)

    1. How can I resolve spray gun clogging during vacuum forming glue application?
    Spray gun clogging is commonly caused by high glue viscosity or impurities. You can reduce thickener content to lower viscosity and re-filter the plastic suction glue with a 200-mesh filter before spraying.
    2. What causes orange peel or surface pitting after film drying?
    This is usually caused by suboptimal spray atomization, excessive glue viscosity, or improper formulation rheology. Adjusting spray gun atomization, using wetting/leveling agents, or gently sanding with fine sandpaper after drying can resolve this issue.
    3. Why does the PVC film fail to attach properly in board grooves?
    This occurs when the vacuum machine does not achieve sufficient suction pressure or when air is trapped by tightly fitted groove edges. Avoid spraying overly thick glue around groove edges and drill 1–2 small exhaust holes at the bottom of the groove if possible.
    4. What is the recommended activation temperature for PVC vacuum forming?
    The film layer temperature should be maintained above 55°C during the blister heating process to ensure adequate thermal activation and prevent edge unsealing or rebound.
    5. How can I prevent edge unsealing and groove rebound during hot summer storage?
    Ensure the board surface is cooled before releasing pressure, increase the heat-resistant resin proportion in the glue formula, or add 2%–5% curing agent for applications demanding high heat resistance.
    6. How does viscosity affect atomization quality in vacuum forming?
    Lowering viscosity improves atomization, resulting in finer droplets, whereas higher viscosity concentrates the spray. For precision control without altering base viscosity, select thickeners that reduce viscosity under high shear.